Data
ASA drying temperature and time
ASA drying temperature is 65–90 °C (149–194 °F) for 4–12 h, from 15 official rows.

That sentence is the span and the median of the tables below, not a new setpoint. Use the product row when the maker lists one temperature.
Softens at (HDT): 103 °C (217 °F) at 0.45 MPa; 97.3–100 °C (207–212 °F) at 1.8 MPa; 94 °C (201 °F), load not stated. Heat resistance dataset.
Full drying dataset · CSV · JSON · Latest row checked 24 October 2026.
| Brand | Product | Drying temperature | Drying time | Source | Checked |
|---|---|---|---|---|---|
| Anycubic | Anycubic ASA | 70–80 °C (158–176 °F) | 8–12 h | Anycubic ASA technical data sheet (v3.0) | 2026-10-18 |
| Bambu Lab | Bambu ASA | 80 °C (176 °F) | 8 h | Bambu Lab ASA technical data sheet | 2026-10-18 |
| Bambu Lab | Bambu ASA Aero | 80 °C (176 °F) | 8 h | Bambu Lab ASA Aero technical data sheet | 2026-10-18 |
| Bambu Lab | Bambu ASA-CF | 80 °C (176 °F) | 8 h | Bambu Lab ASA-CF technical data sheet | 2026-10-18 |
| Creality | Creality ASA (general guidance) | 70–80 °C (158–176 °F) | 8 h | Creality Wiki: Filament Pre-Printing Guide: Drying | 2026-10-18 |
| ELEGOO | ELEGOO ASA (general guidance) | 65–75 °C (149–167 °F) | 4–8 h | ELEGOO Wiki: FDM filament drying and storage guide | 2026-10-18 |
| ELEGOO | ELEGOO ASA-CF | 85 °C (185 °F) | 8 h | ELEGOO US store: ASA-CF | 2026-10-18 |
| Flashforge | Flashforge ASA-CF | 80 °C (176 °F) | 8–12 h | Drying Temperature and Time | Flashforge Wiki | 2026-10-24 |
| Overture | Overture ASA | 75 °C (167 °F) | 7 h | Overture Filament Drying Guide | 2026-10-18 |
| Polymaker | Fiberon ASA-CF08 | 90 °C (194 °F) | 6 h | Fiberon ASA-CF08 TDS V1.0 | 2026-10-21 |
| Polymaker | PolyLite ASA | 70 °C (158 °F) | 7 h | PolyLite ASA TDS EN V5.4 | 2026-10-21 |
| Polymaker | Polymaker ASA | 70 °C (158 °F) | 7 h | Polymaker ASA technical data sheet | 2026-10-18 |
| Prusament | Prusament ASA | 80 °C (176 °F) | 4 h | Prusa Knowledge Base: Drying filament | 2026-10-18 |
| Siraya Tech | Siraya Tech Fibreheart ASA-GF | 70–80 °C (158–176 °F) | 4–6 h | Siraya Tech Fibreheart ASA-GF TDS | 2026-10-18 |
| SUNLU | SUNLU ASA | 80 °C (176 °F) | 6–8 h | SUNLU Wiki: filament parameter table | 2026-10-18 |