Drying dataset
Will my dryer cover this filament?
Published . Updated .
A 50 °C (122 °F) dryer can dry 19 of 236 filaments in our data, mostly PLA.
If you print PETG, ABS, or nylon, the dryer has to reach the highest temperature listed for that material: PETG 80 °C (176 °F), ABS 85 °C (185 °F), nylon 140 °C (284 °F).
Each figure comes from the maker's own drying instructions, and filaments with no temperature are left out.

Looking for a dryer? See dryers you can buy
Each bar is the highest drying temperature the maker published for that material. The dryer can handle every filament in the material only when it reaches that temperature. Fahrenheit is the figure stored with that temperature.
Materials
| Material | Filaments this dryer can handle | Drying temperature range | Needs the most heat | Handles all of them? |
|---|---|---|---|---|
| PLA | 14 of 61 | 45–75 °C (113–167 °F) | Eryone Standard PLA | Not all |
| PETG | 0 of 31 | 55–70 °C (131–158 °F) | Flashforge PETG | Not all |
| ABS | 0 of 18 | 60–85 °C (140–185 °F) | SUNLU ABS | Not all |
| TPU | 1 of 18 | 50–80 °C (122–176 °F) | Anycubic TPU | Not all |
| PC | 0 of 14 | 70–100 °C (158–212 °F) | Creality PC (general guidance) | Not all |
| ASA | 0 of 11 | 65–80 °C (149–176 °F) | Bambu ASA | Not all |
| PA-CF | 0 of 11 | 70–110 °C (158–230 °F) | SUNLU PA6-CF | Not all |
| PLA+ | 2 of 10 | 45–60 °C (113–140 °F) | Polymaker HT-PLA | Not all |
| PA | 0 of 8 | 70–110 °C (158–230 °F) | SUNLU Easy PA | Not all |
| PETG-CF | 0 of 6 | 60–80 °C (140–176 °F) | Siraya Tech Fibreheart PETG-CF Pro | Not all |
| PET-CF | 0 of 5 | 80–120 °C (176–248 °F) | Creality PET-CF (general guidance) | Not all |
| PLA-CF | 1 of 5 | 50–60 °C (122–140 °F) | Creality PLA-CF (general guidance) | Not all |
| PPA | 0 of 5 | 80–100 °C (176–212 °F) | Siraya Tech Fibreheart PPA | Not all |
| PPA-CF | 0 of 4 | 80–140 °C (176–284 °F) | Bambu PPA-CF | Not all |
| ABS-GF | 0 of 3 | 65–80 °C (149–176 °F) | Bambu ABS-GF | Not all |
| ASA-CF | 0 of 3 | 80–90 °C (176–194 °F) | Fiberon ASA-CF08 | Not all |
| PA-GF | 0 of 3 | 80–110 °C (176–230 °F) | SUNLU PA6-GF | Not all |
| PPS | 0 of 2 | 100–140 °C (212–284 °F) | QIDI PPS-CF | Not all |
| PPS-CF | 0 of 2 | 100–120 °C (212–248 °F) | ELEGOO PPS-CF | Not all |
| PVA | 0 of 2 | 75–85 °C (167–185 °F) | PVA | Not all |
| ABS-CF | 0 of 1 | 60–70 °C (140–158 °F) | Siraya Tech Fibreheart ABS-CF Core | Not all |
| ASA-GF | 0 of 1 | 70–80 °C (158–176 °F) | Siraya Tech Fibreheart ASA-GF | Not all |
| HIPS | 0 of 1 | 80 °C (176 °F) | Flashforge HIPS | Not all |
| PA12 | 0 of 1 | 80–100 °C (176–212 °F) | QIDI PA12-CF | Not all |
| PA6-CF | 0 of 1 | 90–100 °C (194–212 °F) | PA6-CF | Not all |
| PC-CF | 0 of 1 | 90 °C (194 °F) | Prusament PC Blend Carbon Fiber | Not all |
| PEI | 0 of 1 | 150 °C (302 °F) | Prusament PEI | Not all |
| PET-GF | 0 of 1 | 100–120 °C (212–248 °F) | Siraya Tech Fibreheart PET-GF | Not all |
| PLA-GF | 0 of 1 | 60 °C (140 °F) | Polymaker HT-PLA-GF | Not all |
| PP-CF/GF | 0 of 1 | 70 °C (158 °F) | Prusament PP Carbon Fiber / Glass Fiber | Not all |
| PPS-GF | 0 of 1 | 100 °C (212 °F) | Fiberon PPS-GF20 | Not all |
| PVB | 1 of 1 | 45 °C (113 °F) | Prusament PVB | Yes |
| TPE | 0 of 1 | 60 °C (140 °F) | eSUN TPE-95A | Not all |
| TPU-GF | 0 of 1 | 50–60 °C (122–140 °F) | Siraya Tech Fibreheart TPU-GF | Not all |
Brands
| Brand | Filaments this dryer can handle | Drying temperature range | Needs the most heat | Handles all of them? |
|---|---|---|---|---|
| Anycubic | 3 of 16 | 45–100 °C (113–212 °F) | PA6-CF | Not all |
| Bambu Lab | 4 of 35 | 50–140 °C (122–284 °F) | Bambu PPA-CF | Not all |
| Creality | 0 of 12 | 50–120 °C (122–248 °F) | Creality PPA-CF (general guidance) | Not all |
| Dancyn 3D Prints | 0 of 1 | 65 °C (149 °F) | PETG HF | Not all |
| ELEGOO | 0 of 15 | 45–120 °C (113–248 °F) | ELEGOO PPS-CF | Not all |
| Eryone | 0 of 1 | 65–75 °C (149–167 °F) | Eryone Standard PLA | Not all |
| eSUN | 3 of 10 | 50–80 °C (122–176 °F) | eSUN ABS series (general guidance) | Not all |
| Flashforge | 2 of 13 | 50–80 °C (122–176 °F) | Flashforge PVA | Not all |
| Overture | 1 of 7 | 50–95 °C (122–203 °F) | Overture Easy Nylon | Not all |
| Polymaker | 0 of 55 | 55–100 °C (131–212 °F) | PolyMide CoPA | Not all |
| Prusament | 3 of 13 | 45–150 °C (113–302 °F) | Prusament PEI | Not all |
| QIDI Tech | 2 of 19 | 50–140 °C (122–284 °F) | QIDI PPS-CF | Not all |
| Siraya Tech | 0 of 13 | 50–120 °C (122–248 °F) | Siraya Tech Fibreheart PET-GF | Not all |
| SUNLU | 1 of 26 | 50–110 °C (122–230 °F) | SUNLU Easy PA | Not all |
Needs the most heat is the filament with the highest drying temperature in that row. The link is the maker's page. Fahrenheit is the figure stored with that temperature. Checked 26 October 2026.